these precipitates was done with double-distilled lukewarm water. This step was
followed by drying the precipitates for 24 h at 70 C. Mortar and pestle was used to
crush and grind the dried mass into fine powders.
23.4.2 Single-Ion-Substituted Nanodimensional Hydroxyapatites
Zinc nitrate tetrahydrate (ZNT, Zn(NO3)2.4H2O, Merck, AR grade) and magnesium
nitrate tetrahydrate (MNT, Mg(NO3)2.4H2O, Merck, AR grade) were used as zinc
and magnesium precursors for synthesizing zinc-substituted nanodimensional
hydroxyapatite
(ZnHA,
Zn0.2Ca9.8(PO4)6OH2)
and
magnesium-substituted
nanodimensional hydroxyapatite (MgHA, Mg0.2Ca0.98(PO4)6OH2), respectively.
1.0 M Solution A was made by adding appropriate amounts of CNT and ZNT or
MNT in the case of ZnHA and MgHA, respectively, and 0.6 M Solution B was made
by adding appropriate amount of KDP.
Europium nitrate pentahydrate (ENP, Eu(NO)3.5H2O, Merck, AR grade) was
used
as
europium
precursor
for
the
synthesis
of
europium-substituted
nanodimensional hydroxyapatite (EuHA, Eu0.2Ca9.8(PO4)6(OH)2). Appropriate
Fig. 23.1 Protocol for the synthesis of nanodimensional hydroxyapatites by sol-gel method